The only tangible evidence you have of a building’s concrete is the handful of cube specimens taken on the day of the pour. Once the column is cast and the formwork struck, you cannot look inside the concrete; taking cores is both expensive and damaging to the structure. So although sampling can look like a formality on site, it is in fact the structure’s quality certificate. A specimen that is taken wrongly, cured badly or labelled incompletely can make sound concrete look weak on paper; the opposite is also possible. How the specimen is taken, how it is stored and what each line of the incoming report means is a process applied in the field that everyone from the site manager to the building inspector needs to know.
Why Samples Are Taken: The Difference Between Design Concrete and Site Concrete
At the ready-mix batching plant, the mix is designed in the laboratory and the class target is met with a certain safety margin. But the concrete arriving on site is shaped by the time spent in the truck mixer, the air temperature, the pump line, any interventions on site and the quality of placing. The sample is what puts this site reality on record. The plant’s own production control is a separate matter; the sample taken on site is the identity of that day’s pour in the structure.
In Türkiye the building inspection system makes this record mandatory. The building inspection body oversees the taking of samples for every pour and their testing at an accredited laboratory; the results go into the building inspection file, and that file is examined during the occupancy permit process. The sample is therefore not merely a technical check but a legal document. Who took it, when, from which mixer and for which element must be on record.
The sample shows that the strength class has been met; it does not tell the whole story of the concrete’s quality. Poor vibration, inadequate curing or a cold joint do not show up in a cube specimen. Because the cube is stored under ideal conditions in the laboratory, it measures the concrete’s potential; the actual strength in the structure depends on workmanship. Knowing this distinction is necessary both to interpret the report correctly and to keep attention on site from being confined to the sample.
We have covered the choice of strength class in Bodrum and the differences between classes separately; you can find which class suits which element in the ready-mix concrete classes article. This article is about how, once the class has been chosen, you prove on site that that class is what actually arrived.
Sampling on Site: Getting It Right Step by Step
Sampling is described in the TS EN 12350 series; on site the procedure runs in this order. When the truck mixer starts discharging, the first concrete to arrive is not taken; it is the portion left at the head of the chute, with a disturbed water and fines content. The last drop is not taken either. Concrete from the middle of the discharge, collected with several shovelfuls and where possible at more than one moment, is gathered in a clean container and mixed. If a pump is in use, the sample is taken where possible from the pump outlet, that is, from the concrete entering the structure.
When the sample is taken, a slump test is also carried out on the same concrete. Slump indicates the consistency of the concrete; if it does not match the consistency class on the delivery ticket, the situation must be recorded before the sample is taken. The concrete temperature is also measured; in the Bodrum summer, as the temperature of the concrete in the truck mixer rises, workability drops and the risk of early setting increases.
Moulds should be steel or rigid plastic, clean and lightly coated with mould oil on the inside. The concrete is placed in the mould in two or three layers; each layer is rodded a set number of times with a tamping rod or compacted with brief vibration. Insufficient compaction leaves voids in the specimen and makes the strength read low; excessive vibration causes segregation. The surface is finished with a trowel and the edges of the mould are wiped clean.
Labelling is the most neglected step. Each specimen is marked with the date and time of the pour, the mixer registration or delivery ticket number, the target concrete class and the element it was placed in (for example, ground-floor columns, second-floor slab). It should be written in indelible marker not on the mould but on a label pressed into the concrete, or on the specimen surface after demoulding. An unlabelled specimen is, in the laboratory, nothing more than a lump of concrete from an unknown pour.
How many specimens are taken is determined by the project and the building inspection procedure; in practice, one set of specimens is taken for each day of pouring, each concrete class and each specified volume interval. The set usually consists of enough cubes for the 7-day and 28-day tests; on some projects spare cubes are set aside as well. The building inspector is present at sampling and signs the record.
Cube or Cylinder? Size and Conversion
The most common specimen on Turkish sites is the 150 mm cube; some laboratories and projects use 150 x 300 mm cylinders. Both are prepared and tested to the TS EN 12390 series. The difference is not only shape but the strength measured. For the same concrete, the cylinder strength comes out lower than the cube strength; the cylinder has a larger height-to-diameter ratio and less end restraint from friction.
The concrete class designation carries this difference. In class C30/37, for example, the first number is the characteristic cylinder strength (30 MPa) and the second the characteristic cube strength (37 MPa). When reading a report, check on the first line whether the specimen is a cube or a cylinder; comparing a cube result that should reach 37 MPa against 30 MPa and taking false comfort is a common mistake. In the reverse case, a sound concrete is unfairly made to look weak.
Cube moulds are easier to handle on site, take up less space and need no additional surface preparation. Cylinders require capping or grinding of the end faces before testing, which is why most sites prefer cubes. Whichever is chosen, it is important to be consistent within the same structure and to state the specimen type clearly in the report.
Specimen size also affects the result. A 100 mm cube gives a somewhat higher strength than a 150 mm cube. A small mould is not suitable for concretes with large aggregate; the general rule is that the mould dimension should be several times the maximum aggregate size. The standard 150 mm cube meets this condition for typical ready-mix concretes.
Curing: The Most Critical 28 Days in a Specimen’s Life
The first 24 hours after sampling are spent on site. During this time the cubes are kept in the shade, free from vibration, out of direct sun and wind, and covered with damp hessian or plastic. A cube left in the open in summer loses water from its surface within a few hours; that lost water leaves hydration incomplete and lowers the strength permanently. In winter there is a risk of freezing; if fresh concrete freezes, the specimen is invalid.
Once demoulded, the specimens are taken to the laboratory and placed in the curing tank. Standard curing is in water at 20 ± 2 °C or in a high-humidity room at the same temperature. Lime-saturated water is generally used so that the tank water does not leach the lime from the concrete. The cubes sit fully submerged in the water, not touching one another. These conditions remain unchanged until the day of testing.
Transport from site to laboratory is as important as curing. The cubes should be moved well before the test date, ideally on the day they are demoulded, protected against vibration. A specimen that sits for a week in the back of a pickup, drying in the sun, has not undergone standard curing; if its result comes out low, the shortfall describes the transport, not the concrete.
The laboratory keeps a record of the curing tank checks: the tank temperature is measured regularly and logged. When a result becomes disputed, this record is the first thing examined. If there is a gap between the date the specimen was demoulded and the date it entered the tank, you are entitled to ask why the report does not say so.
7-Day and 28-Day Testing: What to Expect
Concrete strength increases with time; the acceptance class is defined by the 28-day strength. The 7-day test is there to give an early indication: in concrete made with ordinary Portland cement, the 7-day strength comes out at roughly 65 to 75 per cent of the 28-day strength. The ratio varies with cement type, mineral additions and temperature; in concretes containing fly ash or slag, early strength runs lower and later strength higher.
The real value of the 7-day result is catching problems early. A 7-day value far below expectation is signal enough to start an investigation without waiting for 28 days; formwork striking and loading decisions can also be postponed on the basis of that value. On the other hand, a concrete with a good 7-day value is not guaranteed to meet its class at 28 days; the acceptance decision rests on the 28-day result alone.
Testing is carried out in a calibrated compression machine at the constant loading rate specified in the standard. The specimen is placed on the platen with the cast face to the side; because the cast face is not true, it is not used as a loading face. The maximum load at failure is divided by the specimen’s cross-sectional area to give the strength in MPa.
The failure pattern is also informative. A healthy cube shows a similar, cone-shaped failure on all four faces. One-sided shattering, diagonal shear or a corner breaking off suggests the specimen was not seated properly or its faces were not parallel. Good laboratories note the failure type in the report; when a result comes out abnormal, this note decides whether you question the specimen or the concrete.
Reading the Test Report: Mean, Individual Value, Conformity
The laboratory report has a separate line for each specimen: specimen code, date taken, test date, age, dimensions, weight, density, failure load and strength. Check the date and age first; make sure a result labelled 28 days really was tested at 28 days. Then look at the density; an unusually low density indicates that the specimen was poorly compacted or contains voids.
Two questions are asked in the assessment: does the mean of the specimen group exceed the class’s characteristic strength by an adequate margin, and does the lowest individual value fall below the acceptance limit? The conformity logic of TS EN 206 rests on both conditions being met together. The mean must sit a certain margin above because characteristic strength is a statistical lower bound; for the individual value, a tolerance of a few MPa below the class is allowed. It is wrong to look only at the mean and ignore a single low cube; it is equally wrong to reject the whole pour on account of a single low cube.
The report must make clear the specimen type (cube/cylinder) and which value the class comparison was made against. For C30/37, a 150 mm cube result is compared with 37 MPa. Some reports give a value converted to the cylinder equivalent; in that case the conversion factor must be stated. Reports that compare a cube result with the cylinder class without conversion are misleading.
If there is wide scatter between specimens taken from the same pour, there is a problem even when the average passes. The scatter points either to inconsistent sampling or to concrete that is not homogeneous. In that case the report should be reviewed together with the building inspection body and the sampling procedure tightened for the next pour. The bottom of the report should carry the laboratory’s accreditation details, the name of the person who ran the test and the calibration date of the press; if these are missing, the report will cause problems in the official process.
What to Do If the Result Is Low
A low result is not cause for panic; it is the start of an investigation. The first step is to question the specimen itself: was it taken from the right part of the discharge, how were the first 24 hours handled, when and how was it transported to the laboratory, what does the curing tank record say, is the failure pattern normal? If the answer to any of these is unfavourable, the result tells the story of the specimen, not of the concrete. The spare cubes taken from the same pour come into play at this stage.
If the specimen holds up, the second step is to look at the concrete in the structure. Non-destructive methods (the rebound hammer, which measures surface hardness, and ultrasonic pulse velocity) give a quick idea of the homogeneity and relative quality of the concrete, but do not prove strength on their own. For a definitive result, cores are taken from the structure: cylindrical samples are cut from selected elements, tested in the laboratory, and the results give the actual in-situ strength. Core locations are set with the structural engineer’s approval so as not to cut through reinforcement.
If the core result also falls below the design value, the decision passes to the structural engineer. The engineer recalculates the structure’s load-bearing capacity using the measured strength. In most cases the safety margin in the design absorbs a small strength shortfall and the element is accepted as it is. If the shortfall is large, strengthening (jacketing, fibre-reinforced polymer wrapping) comes onto the agenda. In the most extreme case, the decision is taken to demolish and recast the element. These decisions are recorded together with the building inspection body and the relevant authority.
If the source of the non-conformity lies on site, lessons need to be drawn. The most frequent causes are these: water added to the concrete on site, the truck mixer waiting too long, pouring in high temperatures, inadequate curing. If the cause lies on the plant side, the producer has to account for the process with its own production control records (plant samples from the same day, incoming checks on cement and aggregate). A good ready-mix producer has no hesitation in sharing these records.
Quality on Site Before the Sample: Delivery Ticket, Slump, Water
The sample result arrives 28 days later; yet most quality problems can be seen at the moment of the pour. Read the delivery ticket for every truck mixer that arrives: concrete class, consistency class, maximum aggregate size, admixture details, time of departure from the plant. The time between departure and arrival and discharge on site shows how long the concrete has waited; in hot weather this window shrinks. If the class or consistency does not match the order, call the plant before the mixer is discharged.
The slump test should be done, if not for every mixer, then at least on every day of pouring and whenever there is doubt. If the slump is too high the concrete segregates and strength drops; if too low, placing becomes difficult and voids remain. Adding water on site to correct the consistency is the most common and most damaging habit; every addition of water upsets the water/cement ratio, and if a sample has already been taken, even that sample does not fully reflect it. Consistency is adjusted only with the batching plant’s knowledge, and with a plasticising admixture.
Clarifying responsibility for sampling and testing from the outset when ordering ready-mix concrete prevents disputes between site and plant. Who takes the sample, which laboratory tests it, who receives the result; these should be written into the contract. You are also entitled to ask for the producer’s own quality control results; the difference between plant samples and site samples shows the quality of the work on site.
Around Bodrum and Milas, road and temperature conditions during ready-mix delivery have a direct bearing on sample results. Our group company Bodrum Beton runs this process together with the site by sharing its delivery planning and the quality records for the day of the pour. For your pour schedule and sampling protocol, you can reach us through the contact page.